{"id":1261,"date":"2026-05-12T08:14:06","date_gmt":"2026-05-12T08:14:06","guid":{"rendered":"https:\/\/www.packtests.com\/?post_type=standard&#038;p=1261"},"modified":"2026-05-12T09:09:33","modified_gmt":"2026-05-12T09:09:33","slug":"astm-f1921","status":"publish","type":"standard","link":"https:\/\/www.packtests.com\/pl\/standard\/astm-f1921\/","title":{"rendered":"ASTM F1921"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"1261\" class=\"elementor elementor-1261\" data-elementor-post-type=\"standard\">\n\t\t\t\t<div class=\"elementor-element elementor-element-5ec1237 e-flex e-con-boxed e-con e-parent\" data-id=\"5ec1237\" data-element_type=\"container\">\n\t\t\t\t\t<div class=\"e-con-inner\">\n\t\t\t\t<div class=\"elementor-element elementor-element-b53c995 elementor-widget elementor-widget-text-editor\" data-id=\"b53c995\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t\t\t\t\t\t<h2>Norma ASTM F1921 i metoda badania przyczepno\u015bci na gor\u0105co<\/h2><p>Norma ASTM F1921 okre\u015bla <strong>metoda laboratoryjna s\u0142u\u017c\u0105ca do pomiaru wytrzyma\u0142o\u015bci zgrzew\u00f3w termicznych bezpo\u015brednio po ich utworzeniu<\/strong>, zanim materia\u0142 ostygnie do temperatury otoczenia. Ta w\u0142a\u015bciwo\u015b\u0107 \u2014 znana jako <em>wytrzyma\u0142o\u015b\u0107 na przyczepno\u015b\u0107 na gor\u0105co<\/em>\u2014ma kluczowe znaczenie w \u015brodowiskach pakowania o du\u017cej pr\u0119dko\u015bci, zw\u0142aszcza <strong>formowanie, nape\u0142nianie i zgrzewanie (FFS)<\/strong> procesy.<\/p><p>The <strong>metoda badania przyczepno\u015bci na gor\u0105co<\/strong> symuluje rzeczywiste warunki uszczelniania poprzez poddanie folii termoplastycznych kontrolowanemu dzia\u0142aniu ciep\u0142a i ci\u015bnienia.<\/p><p>W odr\u00f3\u017cnieniu od konwencjonalnych bada\u0144 wytrzyma\u0142o\u015bci uszczelnienia przeprowadzanych w temperaturze pokojowej, norma ASTM F1921 oraz metoda badania przyczepno\u015bci na gor\u0105co pozwalaj\u0105 oceni\u0107 <strong>sprawdzanie integralno\u015bci uszczelnienia w czasie rzeczywistym pod wp\u0142ywem obci\u0105\u017cenia termicznego<\/strong>, co sprawia, \u017ce ma to ogromne znaczenie dla stabilno\u015bci produkcji i niezawodno\u015bci opakowa\u0144.<\/p><h2>Proces badania przyczepno\u015bci na gor\u0105co<\/h2><p>Norma ASTM F1921 okre\u015bla wytrzyma\u0142o\u015b\u0107 zgrzewu bezpo\u015brednio po jego utworzeniu. Cykl badawczy obejmuje zgrzewanie, otwarcie szcz\u0119k, cofni\u0119cie, op\u00f3\u017anienie\/och\u0142odzenie oraz rozdzielenie uchwyt\u00f3w w celu pomiaru si\u0142y.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-ef8e840 e-con-full e-flex e-con e-child\" data-id=\"ef8e840\" data-element_type=\"container\">\n\t\t<div class=\"elementor-element elementor-element-8140b4b e-con-full e-flex e-con e-child\" data-id=\"8140b4b\" data-element_type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-e756c01 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"e756c01\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img fetchpriority=\"high\" decoding=\"async\" width=\"300\" height=\"200\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-1-Seal.webp\" class=\"attachment-large size-large wp-image-1278\" alt=\"Proces badania przyczepno\u015bci na gor\u0105co \u2013 uszczelnienie nr 1\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-1-Seal.webp 300w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-1-Seal-18x12.webp 18w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">1. Piecz\u0119\u0107<\/h3><p class=\"elementor-image-box-description\">Dwa paski s\u0105 zgrzewane w okre\u015blonych warunkach temperatury, ci\u015bnienia i czasu utrzymywania.<\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-4658d39 elementor-widget__width-initial elementor-view-default elementor-widget elementor-widget-icon\" data-id=\"4658d39\" data-element_type=\"widget\" data-widget_type=\"icon.default\">\n\t\t\t\t\t\t\t<div class=\"elementor-icon-wrapper\">\n\t\t\t<div class=\"elementor-icon\">\n\t\t\t<svg aria-hidden=\"true\" class=\"e-font-icon-svg e-fas-long-arrow-alt-right\" viewbox=\"0 0 448 512\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\"><path d=\"M313.941 216H12c-6.627 0-12 5.373-12 12v56c0 6.627 5.373 12 12 12h301.941v46.059c0 21.382 25.851 32.09 40.971 16.971l86.059-86.059c9.373-9.373 9.373-24.569 0-33.941l-86.059-86.059c-15.119-15.119-40.971-4.411-40.971 16.971V216z\"><\/path><\/svg>\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-85446db elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"85446db\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img decoding=\"async\" width=\"300\" height=\"200\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-2-Open-Jaws.webp\" class=\"attachment-large size-large wp-image-1279\" alt=\"Proces badania przyczepno\u015bci na gor\u0105co \u2013 2 szcz\u0119ki otwarte\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-2-Open-Jaws.webp 300w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-2-Open-Jaws-18x12.webp 18w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">2. \u201eOpen Jaws\u201d<\/h3><p class=\"elementor-image-box-description\">Szcz\u0119ki otwieraj\u0105 si\u0119, a obszar uszczelniony zostaje zwolniony.<\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-81869d6 elementor-widget__width-initial elementor-view-default elementor-widget elementor-widget-icon\" data-id=\"81869d6\" data-element_type=\"widget\" data-widget_type=\"icon.default\">\n\t\t\t\t\t\t\t<div class=\"elementor-icon-wrapper\">\n\t\t\t<div class=\"elementor-icon\">\n\t\t\t<svg aria-hidden=\"true\" class=\"e-font-icon-svg e-fas-long-arrow-alt-right\" viewbox=\"0 0 448 512\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\"><path d=\"M313.941 216H12c-6.627 0-12 5.373-12 12v56c0 6.627 5.373 12 12 12h301.941v46.059c0 21.382 25.851 32.09 40.971 16.971l86.059-86.059c9.373-9.373 9.373-24.569 0-33.941l-86.059-86.059c-15.119-15.119-40.971-4.411-40.971 16.971V216z\"><\/path><\/svg>\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-82dcd8d elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"82dcd8d\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img decoding=\"async\" width=\"300\" height=\"200\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-3-Withdraw.webp\" class=\"attachment-large size-large wp-image-1280\" alt=\"Proces badania przyczepno\u015bci na gor\u0105co, etap 3: Wycofanie\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-3-Withdraw.webp 300w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-3-Withdraw-18x12.webp 18w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">3. Wyp\u0142ata<\/h3><p class=\"elementor-image-box-description\">Pr\u00f3bka jest automatycznie wyjmowana z zacisk\u00f3w.<\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-3657b98 e-con-full e-flex e-con e-child\" data-id=\"3657b98\" data-element_type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-e93267b elementor-widget__width-initial elementor-view-default elementor-widget elementor-widget-icon\" data-id=\"e93267b\" data-element_type=\"widget\" data-widget_type=\"icon.default\">\n\t\t\t\t\t\t\t<div class=\"elementor-icon-wrapper\">\n\t\t\t<div class=\"elementor-icon\">\n\t\t\t<svg aria-hidden=\"true\" class=\"e-font-icon-svg e-fas-long-arrow-alt-right\" viewbox=\"0 0 448 512\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\"><path d=\"M313.941 216H12c-6.627 0-12 5.373-12 12v56c0 6.627 5.373 12 12 12h301.941v46.059c0 21.382 25.851 32.09 40.971 16.971l86.059-86.059c9.373-9.373 9.373-24.569 0-33.941l-86.059-86.059c-15.119-15.119-40.971-4.411-40.971 16.971V216z\"><\/path><\/svg>\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-17acaff elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"17acaff\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"300\" height=\"200\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-4-Delay-Cooling.webp\" class=\"attachment-large size-large wp-image-1281\" alt=\"Proces badania przyczepno\u015bci na gor\u0105co, etap 4: ch\u0142odzenie z op\u00f3\u017anieniem\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-4-Delay-Cooling.webp 300w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-4-Delay-Cooling-18x12.webp 18w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">4. Op\u00f3\u017anienie \/ Ch\u0142odzenie<\/h3><p class=\"elementor-image-box-description\">Po otwarciu szcz\u0119k rozpoczyna si\u0119 ustalony czas op\u00f3\u017anienia (czas ch\u0142odzenia).<\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e6530af elementor-widget__width-initial elementor-view-default elementor-widget elementor-widget-icon\" data-id=\"e6530af\" data-element_type=\"widget\" data-widget_type=\"icon.default\">\n\t\t\t\t\t\t\t<div class=\"elementor-icon-wrapper\">\n\t\t\t<div class=\"elementor-icon\">\n\t\t\t<svg aria-hidden=\"true\" class=\"e-font-icon-svg e-fas-long-arrow-alt-right\" viewbox=\"0 0 448 512\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\"><path d=\"M313.941 216H12c-6.627 0-12 5.373-12 12v56c0 6.627 5.373 12 12 12h301.941v46.059c0 21.382 25.851 32.09 40.971 16.971l86.059-86.059c9.373-9.373 9.373-24.569 0-33.941l-86.059-86.059c-15.119-15.119-40.971-4.411-40.971 16.971V216z\"><\/path><\/svg>\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f33db0e elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"f33db0e\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"300\" height=\"200\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-5-Separate-Measure.webp\" class=\"attachment-large size-large wp-image-1282\" alt=\"Proces badania przyczepno\u015bci na gor\u0105co \u2013 etap 5: Oddzielenie i pomiar\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-5-Separate-Measure.webp 300w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Hot-Tack-Testing-Process-5-Separate-Measure-18x12.webp 18w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">5. Oddziel i odmierz<\/h3><p class=\"elementor-image-box-description\">Uchwyty s\u0105 rozdzielane ze sta\u0142\u0105 pr\u0119dko\u015bci\u0105, a si\u0142a potrzebna do roz\u0142\u0105czenia uszczelnienia jest mierzona a\u017c do momentu jego uszkodzenia.<\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c1d4788 elementor-widget elementor-widget-text-editor\" data-id=\"c1d4788\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t\t\t\t\t\t<h2>Kluczowe zmienne w badaniach zgodnie z norm\u0105 ASTM F1921<\/h2><ul><li><strong>Temperatura uszczelniania:<\/strong> Zazwyczaj modyfikowana w celu uzyskania krzywej przyczepno\u015bci na gor\u0105co<\/li><li><strong>Czas przebywania:<\/strong><ul><li>Warstwy o grubo\u015bci \u226425 \u00b5m: ~0,5 s<\/li><li>Warstwy o grubo\u015bci 25\u201364 \u00b5m: ~1,0 s<\/li><li>Warstwy o grubo\u015bci 64 \u00b5m: ~2,5 s<\/li><\/ul><\/li><li><strong>Ci\u015bnienie uszczelniaj\u0105ce:<\/strong> 15\u201330 N\/cm\u00b2<\/li><li><strong>Czas ch\u0142odzenia \/ czas op\u00f3\u017anienia:<\/strong> Okre\u015bla harmonogram pomiar\u00f3w<\/li><li><strong>Pr\u0119dko\u015b\u0107 separacji:<\/strong> Zazwyczaj 200 mm\/min (metoda A)<\/li><\/ul><p>Parametry te maj\u0105 bezpo\u015bredni wp\u0142yw na wynik <strong>wytrzyma\u0142o\u015b\u0107 zgrzewu opakowa\u0144 elastycznych<\/strong> materia\u0142y.<\/p><h2>Tester przyczepno\u015bci na gor\u0105co: niezb\u0119dny sprz\u0119t do bada\u0144 zgodnie z norm\u0105 ASTM F1921<\/h2><p>A <strong>urz\u0105dzenie do badania przyczepno\u015bci na gor\u0105co<\/strong> zosta\u0142 specjalnie zaprojektowany w celu odtworzenia procesu zgrzewania i natychmiastowego odrywania okre\u015blonego w normie ASTM F1921. Zaawansowane systemy \u2014 takie jak te opracowane przez firm\u0119 Cell Instruments Co., Ltd. \u2014 oferuj\u0105:<\/p><ul><li><strong>Systemy sterowania oparte na sterownikach PLC<\/strong> w celu zapewnienia powtarzalno\u015bci<\/li><li><strong>Regulacja temperatury metod\u0105 PID (dok\u0142adno\u015b\u0107 \u00b10,2 \u00b0C)<\/strong><\/li><li><strong>Zautomatyzowane cykle testowe<\/strong> wyeliminowanie wp\u0142ywu operatora<\/li><li><strong>Regulowane pr\u0119dko\u015bci i ci\u015bnienia testowe<\/strong><\/li><li><strong>Pomiar si\u0142y w wysokiej rozdzielczo\u015bci<\/strong><\/li><\/ul>\t\t\t\t\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-696a839 e-con-full e-flex e-con e-child\" data-id=\"696a839\" data-element_type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-a44a8e6 elementor-widget elementor-widget-text-editor\" data-id=\"a44a8e6\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t\t\t\t\t\t<h3>Zalecane rozwi\u0105zanie<\/h3><p>Seria Cell Instruments HTT obs\u0142uguje:<\/p><ul><li><strong>Metoda A (sta\u0142e op\u00f3\u017anienie)<\/strong> oraz <strong>Metoda B (zmienne op\u00f3\u017anienie)<\/strong><\/li><li>R\u00f3\u017cne tryby testowania: przyczepno\u015b\u0107 na gor\u0105co, odrywanie, rozci\u0105ganie, zgrzewanie<\/li><li>Testy przy du\u017cych pr\u0119dko\u015bciach do <strong>12 000 mm\/min<\/strong> (HTT-02)<\/li><\/ul><p>Ta elastyczno\u015b\u0107 pozwala na precyzyjn\u0105 charakterystyk\u0119 r\u00f3\u017cnych materia\u0142\u00f3w i ich w\u0142a\u015bciwo\u015bci uszczelniaj\u0105cych.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1d56d80 elementor-widget elementor-widget-image\" data-id=\"1d56d80\" data-element_type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img loading=\"lazy\" decoding=\"async\" width=\"400\" height=\"638\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/ASTM-F1921-Hot-Tack-Tester.webp\" class=\"attachment-large size-large wp-image-1283\" alt=\"Tester przyczepno\u015bci na gor\u0105co zgodny z norm\u0105 ASTM F1921\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/ASTM-F1921-Hot-Tack-Tester.webp 400w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/ASTM-F1921-Hot-Tack-Tester-188x300.webp 188w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/ASTM-F1921-Hot-Tack-Tester-8x12.webp 8w\" sizes=\"(max-width: 400px) 100vw, 400px\" title=\"\">\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-c31033e elementor-widget elementor-widget-text-editor\" data-id=\"c31033e\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t\t\t\t\t\t<h2><strong>Wytrzyma\u0142o\u015b\u0107 po\u0142\u0105cze\u0144 termicznych opakowa\u0144 elastycznych<\/strong><\/h2><p>The <strong>wytrzyma\u0142o\u015b\u0107 zgrzewu opakowa\u0144 elastycznych<\/strong> okre\u015bla, czy opakowanie jest w stanie wytrzyma\u0107 obci\u0105\u017cenia bezpo\u015brednio po zamkni\u0119ciu. S\u0142aba przyczepno\u015b\u0107 na gor\u0105co mo\u017ce prowadzi\u0107 do:<\/p><ul><li>Otwarcie uszczelki podczas nape\u0142niania<\/li><li>Zanieczyszczenie produktu lub wyciek<\/li><li>Obni\u017cona wydajno\u015b\u0107 pakowania<\/li><li>Wzrost ilo\u015bci odpad\u00f3w i przestoj\u00f3w<\/li><\/ul><p>Norma ASTM F1921 pomaga producentom:<\/p><ul><li><strong>Ocena w\u0142a\u015bciwo\u015bci materia\u0142u<\/strong><\/li><li><strong>Zoptymalizuj parametry uszczelnienia<\/strong><\/li><li><strong>Zapewnienie niezawodno\u015bci proces\u00f3w w operacjach FFS<\/strong><\/li><\/ul><h2>Metody badawcze zgodne z norm\u0105 ASTM F1921<br \/>\u2014Metoda A a metoda B<\/h2><p>Norma ASTM F1921 okre\u015bla dwa odr\u0119bne podej\u015bcia:<\/p><h3>Metoda A \u2013 Sta\u0142e op\u00f3\u017anienie<\/h3><ul><li>Mierzy wytrzyma\u0142o\u015b\u0107 uszczelnienia przy <strong>okre\u015blone czasy ch\u0142odzenia<\/strong><\/li><li>Tworzy <strong>Krzywa zale\u017cno\u015bci wytrzyma\u0142o\u015bci przy zgrzewaniu na gor\u0105co od czasu<\/strong><\/li><li>Nadaje si\u0119 do szczeg\u00f3\u0142owej analizy zachowania uk\u0142adu ch\u0142odzenia<\/li><\/ul><h3>Metoda B \u2013 Op\u00f3\u017anienie zmienne<\/h3><ul><li>\u015arodki <strong>maksymalna si\u0142a po up\u0142ywie wybranego czasu op\u00f3\u017anienia<\/strong><\/li><li>Szybsze i prostsze rutynowe badania kontroli jako\u015bci<\/li><li>Idealny do <strong>\u015brodowiska produkcyjne<\/strong><\/li><\/ul><h2>Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d<\/h2><p>Aby prawid\u0142owo zinterpretowa\u0107 wyniki badania zgodnie z norm\u0105 ASTM F1921, niezb\u0119dna jest znajomo\u015b\u0107 rodzaj\u00f3w odrywania uszczelki. R\u00f3\u017cne rodzaje uszkodze\u0144 wskazuj\u0105 na r\u00f3\u017cne problemy zwi\u0105zane z materia\u0142em lub procesem.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t<div class=\"elementor-element elementor-element-63ec2a0 e-con-full e-flex e-con e-child\" data-id=\"63ec2a0\" data-element_type=\"container\">\n\t\t<div class=\"elementor-element elementor-element-b7ab802 e-con-full e-grid e-con e-child\" data-id=\"b7ab802\" data-element_type=\"container\">\n\t\t\t\t<div class=\"elementor-element elementor-element-34fc5c5 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"34fc5c5\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-1.webp\" class=\"attachment-large size-large wp-image-1284\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 1\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-1.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-1-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Odklejanie kleju<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">Do rozdzielenia dochodzi na granicy mi\u0119dzy dwiema powierzchniami.<br><b>Oznacza: <\/b>S\u0142abe wi\u0105zanie mi\u0119dzyfazowe lub niewystarczaj\u0105ca temperatura\/ci\u015bnienie.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-9691fc8 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"9691fc8\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-2.webp\" class=\"attachment-large size-large wp-image-1285\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 2\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-2.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-2-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Peeling sp\u00f3jny<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">Uszkodzenie wyst\u0119puje w jednej z warstw polimerowych.<br><b>Oznacza:<\/b> Silne wi\u0105zanie mi\u0119dzyfazowe; sam materia\u0142 ulega zniszczeniu.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-b8ab6b4 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"b8ab6b4\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-3.webp\" class=\"attachment-large size-large wp-image-1286\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 3\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-3.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-3-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Rozwarstwienie<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">Odst\u0119p mi\u0119dzy warstwami struktury wielowarstwowej. <br><b>Oznacza:<\/b> S\u0142abe wi\u0105zanie mi\u0119dzy warstwami w materia\u0142ach laminowanych.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-90ba3b6 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"90ba3b6\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-4.webp\" class=\"attachment-large size-large wp-image-1287\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 4\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-4.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-4-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Przerwa na posi\u0142ek<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">Film pokazuje obszar poza stref\u0105 uszczelnienia<br><b>Oznacza:<\/b> Uszczelnienie jest trwalsze ni\u017c pod\u0142o\u017ce.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-f67fd38 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"f67fd38\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-5.webp\" class=\"attachment-large size-large wp-image-1288\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 5\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-5.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-5-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Zdalne wy\u0142\u0105czenie<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">P\u0119kni\u0119cie wyst\u0119puje w miejscu oddalonym od uszczelki.<br><b>Oznacza:<\/b> Uszczelka jest znacznie wytrzymalsza ni\u017c sam materia\u0142.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-b467121 elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"b467121\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-6.webp\" class=\"attachment-large size-large wp-image-1289\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 6\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-6.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-6-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Wyd\u0142u\u017cenie materia\u0142u<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">Materia\u0142 bez uszczelnienia ulega znacznemu rozci\u0105gni\u0119ciu przed zerwaniem.<br><b>Oznacza:<\/b> Wysoka plastyczno\u015b\u0107 i elastyczno\u015b\u0107 folii.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-17b150b elementor-widget__width-inherit elementor-position-top elementor-widget elementor-widget-image-box\" data-id=\"17b150b\" data-element_type=\"widget\" data-widget_type=\"image-box.default\">\n\t\t\t\t\t<div class=\"elementor-image-box-wrapper\"><figure class=\"elementor-image-box-img\"><img loading=\"lazy\" decoding=\"async\" width=\"162\" height=\"122\" src=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-7.webp\" class=\"attachment-large size-large wp-image-1290\" alt=\"Rodzaje uszkodze\u0144 w badaniach metod\u0105 \u201ehot tack\u201d 7\" title=\"\" srcset=\"https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-7.webp 162w, https:\/\/www.packtests.com\/wp-content\/uploads\/2026\/05\/Failure-Modes-in-Hot-Tack-Testing-7-16x12.webp 16w\" sizes=\"(max-width: 162px) 100vw, 162px\" \/><\/figure><div class=\"elementor-image-box-content\"><h3 class=\"elementor-image-box-title\">Odrywanie przy wyd\u0142u\u017ceniu<\/h3><p class=\"elementor-image-box-description\"><p style=\"text-align: left\">Odwarstwianie, kt\u00f3remu towarzyszy znaczne wyd\u0142u\u017cenie nieuszczelnionego materia\u0142u.<br><b>Oznacza:<\/b> Po\u0142\u0105czenie uszkodzenia spoiny klejowej i plastyczno\u015bci materia\u0142u.<\/p><\/p><\/div><\/div>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-544c157 elementor-widget elementor-widget-text-editor\" data-id=\"544c157\" data-element_type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t\t\t\t\t\t<h2>Tworzenie krzywej \u201ehot tack\u201d w celu optymalizacji procesu<\/h2><p>A <strong>krzywa przyczepno\u015bci na gor\u0105co<\/strong> przedstawia zale\u017cno\u015b\u0107 wytrzyma\u0142o\u015bci uszczelnienia od temperatury. Pomaga to okre\u015bli\u0107:<\/p><ul><li>Temperatura inicjacji uszczelnienia (SIT)<\/li><li>Okno o optymalnej szczelno\u015bci<\/li><li>Maksymalna wytrzyma\u0142o\u015b\u0107 na odrywanie na gor\u0105co<\/li><\/ul><p>Dane te pozwalaj\u0105 in\u017cynierom na <strong>dostosowa\u0107 parametry uszczelniania w celu zapewnienia sta\u0142ej wydajno\u015bci pakowania<\/strong>.<\/p><h2>Najcz\u0119\u015bciej zadawane pytania dotycz\u0105ce normy ASTM F1921<\/h2><ol><li><strong> Jaki jest g\u0142\u00f3wny cel normy ASTM F1921?<\/strong><br \/>Ocenia to <strong>wytrzyma\u0142o\u015b\u0107 na odrywanie termoplastycznych uszczelek bezpo\u015brednio po zgrzaniu<\/strong>, zapewniaj\u0105c niezawodno\u015b\u0107 opakowa\u0144 podczas produkcji.<\/li><li><strong> Czym norma ASTM F1921 r\u00f3\u017cni si\u0119 od normy ASTM F88?<\/strong><br \/><a href=\"https:\/\/store.astm.org\/f1921_f1921m-12r23.html\" target=\"_blank\" rel=\"noopener nofollow\">ASTM F1921<\/a> \u015brodki <strong>wytrzyma\u0142o\u015b\u0107 zgrzewu na gor\u0105co<\/strong>, podczas gdy norma ASTM F88 okre\u015bla <strong>wytrzyma\u0142o\u015b\u0107 po\u0142\u0105czenia na zimno<\/strong> po ostygni\u0119ciu.<\/li><li><strong> W jakich bran\u017cach stosuje si\u0119 testy przyczepno\u015bci na gor\u0105co?<\/strong><br \/>Bran\u017ce spo\u017cywcza, farmaceutyczna, wyrob\u00f3w medycznych oraz opakowa\u0144 elastycznych w znacznym stopniu opieraj\u0105 si\u0119 na tym badaniu.<\/li><li><strong> Jaka jest r\u00f3\u017cnica mi\u0119dzy metod\u0105 A a metod\u0105 B?<\/strong><br \/>Metoda A mierzy si\u0142\u0119 w funkcji czasu; metoda B rejestruje maksymaln\u0105 si\u0142\u0119 po up\u0142ywie okre\u015blonego czasu.<\/li><li><strong> Dlaczego przyczepno\u015b\u0107 na gor\u0105co ma znaczenie w procesach FFS?<\/strong><br \/>Poniewa\u017c uszczelki s\u0105 nara\u017cone na obci\u0105\u017cenia przed sch\u0142odzeniem, niewystarczaj\u0105ca przyczepno\u015b\u0107 na gor\u0105co mo\u017ce spowodowa\u0107 <strong>uszkodzenie uszczelki podczas pakowania<\/strong>.<\/li><\/ol>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>ASTM F1921 and Hot Tack Test Method ASTM F1921 defines a laboratory method for measuring the strength of heat seals immediately after formation, before the material cools to ambient temperature. This property\u2014known as hot tack strength\u2014is critical in high-speed packaging environments, especially form-fill-seal (FFS) processes. The hot tack test method simulates actual sealing conditions by [&hellip;]<\/p>","protected":false},"featured_media":0,"parent":0,"template":"","meta":{"_acf_changed":false},"standard-category":[64],"class_list":["post-1261","standard","type-standard","status-publish","hentry","standard-category-astm"],"acf":[],"_links":{"self":[{"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/standard\/1261","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/standard"}],"about":[{"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/types\/standard"}],"version-history":[{"count":5,"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/standard\/1261\/revisions"}],"predecessor-version":[{"id":1297,"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/standard\/1261\/revisions\/1297"}],"wp:attachment":[{"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/media?parent=1261"}],"wp:term":[{"taxonomy":"standard-category","embeddable":true,"href":"https:\/\/www.packtests.com\/pl\/wp-json\/wp\/v2\/standard-category?post=1261"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}